6063-T5 vs T6 Aluminum Windows: Profile Comparison
For 6063 architectural mill-finish profiles, GB/T 5237.1-2017 Table 12 specifies minimum tensile/proof strengths of 160/110 MPa for T5 and 205/180 MPa for T6. Select T6 when material strength controls the design, and select adequate section inertia and supports when elastic deflection controls. GB/T 5237.1 source record
How do T5 and T6 change the same 6063 alloy?
6063-T5 is cooled from hot shaping and artificially aged, while 6063-T6 is solution heat-treated and artificially aged.
The alloy number identifies the material composition, and the temper identifies its processing condition. Architectural extrusions in either temper can be supplied for window frames. Keeping 6063 fixed makes the material comparison meaningful. A quotation for 6060-T66 introduces a different alloy as well as a different temper.
Artificial ageing develops the specified material properties through a controlled production route. A producer technical sheet notes that T6 properties may be obtained through press quenching. The temper designation alone leaves the detailed processing schedule to the qualified production route.
For formed or welded members, include the fabrication sequence in the selection. Welding can reduce T6 strength in the weld region. Both T5 and T6 are used for anodized architectural surfaces, with the finish specified alongside the extrusion.
What changes between 6063-T5 and T6 in the 2017 GB table?
| Property in GB/T 5237.1-2017 Table 12 | 6063-T5 | 6063-T6 |
|---|---|---|
| Minimum tensile strength Rm | 160 MPa | 205 MPa |
| Minimum 0.2% proof strength Rp0.2 | 110 MPa | 180 MPa |
| Minimum elongation A / A50 mm | 8% / 8% | 8% / 8% |
| Wall-thickness entry | All within this profile standard | All within this profile standard |
Identical profile outlines carry separate strength minima and an equal-E elastic model.
How much higher is the T6 strength minimum?
Under GB/T 5237.1-2017 Table 12, the 6063-T6 proof-strength minimum is 70 MPa higher than T5, an increase of 63.6%. The tensile-strength minimum rises by 45 MPa, or 28.1%.
The GB/T 5237.1-2017 architectural-profile standard applies these rows to room-temperature longitudinal tensile tests on mill-finish profiles. Its thickness cell reads “all” for both 6063-T5 and T6. The material minima become inputs to the structural design, which also considers member geometry, connections and the applicable design method.
GB/T 5237.1-2017 Table 12 gives both 6063-T5 and T6 minimum elongation of 8% in each of its A and A50 mm columns. Each elongation column retains its own specimen basis. Match the reported test method and column when reviewing a material certificate.
Why do North American and European figures differ?
One North American extruder's June 2026 sheet gives T5 tensile/proof minima of 22/16 ksi (150/110 MPa) and T6 minima of 30/25 ksi (205/170 MPa) for the shared thickness band up to 3.20 mm. Its T5 row extends to 12.50 mm. The parenthesized metric values follow the sheet's rounded entries.
The same sheet uses the wall thickness where the tensile specimen is taken. Its 8% elongation entries use a 2-inch gauge length or four specimen diameters. The elongation test is exempted for shapes thinner than 0.062 inch and shapes too small for a standard specimen.
BSI lists BS EN 755-2:2025 as the current edition, replacing BS EN 755-2:2016. A material order for a British project should identify the applicable edition and extruded product form. Earlier producer tables that cite the 2016 edition retain that historical basis.
The 0.8 mm lower limit sits beside the hardness specimen.
Will changing to T6 make the same section stiffer?
One European extruder's 2023 data sheet gives 6063 a typical elastic modulus of 69 GPa at 20°C, and elastic beam calculations use section stiffness EI. The modulus entry is an alloy-wide typical value.
The University of Arizona beam equations express elastic deflection through load, span, support conditions and EI. E is the material’s elastic modulus. I describes how the cross-section distributes metal around its bending axis. An increase in I reduces elastic movement under otherwise fixed conditions.
The 63.6% proof-strength difference belongs in the strength assessment. Under equal E, section geometry, load, span and supports, both tempers give the same calculated elastic deflection. A member that bends too far needs a review of section inertia, span or restraint. Actual window movement, wind resistance and U-factor require the complete configuration’s calculations or test results.
The window-profile thickness guide examines wall thickness and frame depth. Put those dimensions beside the temper on the same section drawing. Use the aluminium-window thermal performance guide for the frame, glass and insulating connection.
For a matched-section elastic calculation using E = 69 GPa for both tempers, the T6/T5 stiffness ratio is 1.00. Equal E is the calculation assumption. Keep the chamber geometry, local walls and bending axis identical when evaluating this ratio.
| Assumptions: same load, span and supports | 6063-T5 | 6063-T6 |
|---|---|---|
| Assumed elastic modulus E | 69 GPa | 69 GPa |
| Normalized section inertia I | 1.00 | 1.00 |
| Normalized elastic stiffness EI | 1.00 | 1.00 |
What do batch testing and hardness actually establish?
For mechanical testing, GB/T 5237.1-2017 Table 15 selects 2 profiles per heat-treatment batch and 1 specimen from each profile. Clause 6.2 groups a batch by the same alloy, temper and dimensional specification. The material certificate can therefore be matched to the supplied section and production batch.
For 6063-T5, Table 12 lists a minimum hardness-specimen thickness of 0.8 mm and reference hardness HV 58 and HW 8. The “not less than” heading covers the specimen-thickness column. The T6 hardness cells contain dashes.
Clause 4.5 requires the room-temperature longitudinal tensile results to meet Table 12 and gives hardness for reference. Tensile strength, 0.2% proof strength and elongation therefore belong in the material acceptance record, with their own test basis.
A hardness reading can assist production screening. Acceptance of the specified tensile, proof-strength and elongation values uses the corresponding tensile-test results. Record the actual specimen dimensions and method with those results, especially when comparing certificates prepared under different specifications.
FAQ
Is 6063-T6 always the better choice for windows?
T6 offers a higher material-strength minimum, with 180 MPa proof strength under GB/T 5237.1-2017. Choose it when the section’s strength assessment benefits from that level. Geometry, supports and fabrication remain part of the selection.
Does 6063-T6 have lower minimum elongation than T5?
Both have 8% minimum elongation in the A and A50 mm columns of GB/T 5237.1-2017 Table 12. Other specifications can use different thickness bands and specimen bases.
Which values belong to a 6063-T5 versus T6 comparison?
Use the same alloy, product form and specification. The 2017 GB rows give 6063-T5/T6 tensile minima of 160/205 MPa. A 6060-T66 offer changes both the alloy and temper, so it requires its own material row.
Is a Webster hardness reading enough to accept T6 profiles?
Table 12 gives 6063-T5 reference HW 8 with a hardness specimen at least 0.8 mm thick and leaves the T6 hardness entry blank. Clause 4.5 bases compliance on the specified longitudinal tensile results, including proof strength and elongation.